XF-202Q features high-temperature resistance (able to withstand 150ºC baking for 240 hours, flame retardancy meeting UL-941.6mm V0), precipitation resistance, and can be used for glass fiber reinforced modified PP. It is suitable for use as corrugated pipe material.
Experimental Formulations
Experimental Formulations
| Formula | Copolymerized PP | XF-202Q | Talcum | EBS | 168 | 1010 |
| #1 | 96.7 | 2.8 | / | 0.20 | 0.20 | 0.10 |
| #2 | 86.5 | 3 | 10 | 0.20 | 0.20 | 0.10 |
After blending XF-202Q with PP, the extrusion temperature is 170ºC~190ºC, and the injection temperature is 200ºC~210ºC. The performance is as follows:
| Index | Test Method | Unit | Result | #1 | #2 |
| Flame Retardancy | UL94 | 3.2 mm | NG | V-2 | V-2 |
| 1.6 mm | NG | V-2 | V-2 | ||
| UL94 (150°C, 24h) | 3.2 mm | V-2 | V-2 | ||
| 1.6 mm | V-2 | V-2 | |||
| GWIT | 3.2 mm | NG | 750°C | 750°C | |
| GWFI | 3.2 mm | NG | 850°C | 850°C |